ASME B16.5-2020 vs 2003: What Changed for Nickel Alloy Flanges

What changed between ASME B16.5-2003 and ASME B16.5-2020 for Group 3.8 nickel alloys

The pressure-temperature numbers did not change. The material notes did, and they changed in a way that is easy to misread. ASME B16.5-2020 renumbered the notes under Table 2-3.8 for Group 3.8 materials, so a note reference carried over from a 2003 purchase order can now point at a different rule. Below is the comparison, read from the 2020 tables themselves and checked line by line against the 2003 edition.

The pressure-temperature tables are unchanged

Table 2-3.8 in the 2020 edition gives working pressures in bar and Table 2-3.8C gives the same ratings in psig. Both were compared cell by cell against the corresponding 2003 tables: 161 bar cells and 140 psig cells, with no differences. If you are selecting a class for a given temperature, the answer is the same in either edition.

The notes were renumbered

This is the part that catches people out. The 2020 edition keeps eight notes, but their contents have shifted position relative to 2003.

NoteASME B16.5-2003ASME B16.5-2020
(1)Use solution annealed material only.Use solution annealed material only.
(2)Not to be used over 675°C.Not to be used over 675°C.
(3)Use annealed material only.Use annealed material only.
(4)Not to be used over 645°C. Alloy N06625 in the annealed condition is subject to severe loss of impact strength at room temperatures after exposure in the range of 538°C to 760°C.Not to be used over 645°C. Alloy N06625 in the annealed condition is subject to severe loss of impact strength at room temperatures after exposure in the range of 538°C to 760°C.
(5)Not to be used over 425°C.Grade 1.
(6)The chemical composition, mechanical properties, heat treating requirements, and grain size requirements shall conform to the applicable ASTM specification. The manufacturing procedures, tolerances, tests, certification, and markings shall be in accordance with ASTM B 564.Not to be used over 425°C.
(7)Not to be used over 538°C.Not to be used over 538°C.
(8)Alloy N06022 in the solution annealed condition is subject to severe loss of impact strength at room temperature after exposure to temperatures in the range of 538°C to 675°C.Alloy N06022 in the solution annealed condition is subject to severe loss of impact strength at room temperature after exposure to temperatures in the range of 538°C to 675°C.

Two consequences follow. First, the 425°C service limit that 2003 called note (5) is note (6) in the 2020 edition, so a specification that cites “note (5)” by number alone now means something different. Second, the 2003 note (6), which required the chemical composition, mechanical properties, heat treatment and grain size to conform to the applicable ASTM specification with manufacturing, tolerances, tests, certification and markings in accordance with ASTM B 564, is not present as a numbered note in the 2020 table. It is replaced by a short new note (5) reading “Grade 1.”

Grade 1 is now a numbered note of its own

The new note (5) is short but it is not cosmetic. It is attached to the Alloy 625 rows, and it appears on the 2020 entries for UNS N06625 as B564 Gr. N06625 and B443 Gr. N06625. The 2003 edition listed those grades against notes (3) and (4) only. Note (3), “Use annealed material only”, is unchanged; note (4), the 645°C limit with the impact-strength warning for annealed N06625 between 538°C and 760°C, is unchanged as well. What is new is the grade requirement attached alongside them.

This matters because Alloy 625 is supplied in more than one condition. ASME SB-443 and ASME SB-444 both cover the grade, and the delivery condition affects the mechanical properties. A note that names the grade in the table means the grade is no longer left to the purchase order to settle.

Three forged forms are no longer listed

In the 2003 edition, three of the Group 3.8 rows carried a forging entry that the 2020 edition replaces with an ellipsis, meaning the row is not offered in that product form.

Nominal designation2003 forging entry2020 forging entry
62Ni-28Mo-5FeB 335 Gr. N10001 (1), (2), (5)…
70Ni-16Mo-7Cr-5FeB 573 Gr. N10003 (6), (3)…
61Ni-16Mo-16CrB 574 Gr. N06455 (1), (6), (5)…

These are the nickel-molybdenum and nickel-molybdenum-chromium-iron rows, and the low-carbon nickel-chromium-molybdenum row. The corresponding plate entries survive, and each of them picks up the renumbered note reference: N10001 and N06455 carry note (6) in the 2020 plate column where they carried note (5) in 2003, and N06200 does the same in both its forging and plate columns.

Full side-by-side comparison

Every row of the 2020 Group 3.8 table, with the 2003 entries beneath it for reference.

Nominal designation2003 Forgings2020 Forgings2020 Castings2020 Plates
54Ni-16Mo-15CrB 462 Gr. N10276 (1), (2)B462 Gr. N10276 (1), (2)…B575 Gr. N10276 (1), (2)
60Ni-22Cr-9Mo-3.5CbB 564 Gr. N06625 (3), (4)B564 Gr. N06625 (3)-(5)…B443 Gr. N06625 (3)-(5)
62Ni-28Mo-5FeB 335 Gr. N10001 (1), (2), (5)……B333 Gr. N10001 (1), (6)
70Ni-16Mo-7Cr-5FeB 573 Gr. N10003 (6), (3)……B434 Gr. N10003 (3)
61Ni-16Mo-16CrB 574 Gr. N06455 (1), (6), (5)……B575 Gr. N06455 (1), (6)
42Ni-21.5Cr-3Mo-2.3CuB 564 Gr. N08825 (3), (7)B564 Gr. N08825 (3), (7)…B424 Gr. N08825 (3), (7)
55Ni-21Cr-13.5MoB 462 Gr. N06022 (1), (2), (8)B462 Gr. N06022 (1), (2), (8)…B575 Gr. N06022 (1), (2), (8)
55Ni-23Cr-16Mo-1.6CuB 462 Gr. N06200 (1), (5)B462 Gr. N06200 (1), (6)…B575 Gr. N06200 (1), (6)

The 2003 material block has no separate castings column populated for these rows, so the castings column is shown for the 2020 edition only, with the ellipsis that ASME prints where a form is not listed.

Why this matters when you order

Two practical consequences for anyone specifying nickel alloy flanges against a 2003-era drawing or a supplier quotation written before the 2020 edition came out.

  • Do not carry a note number across editions. Write the requirement out, or state the edition of B16.5 you are ordering to. A bare “note (5)” means one thing in 2003 and something else in 2020.
  • Check the delivery condition for Alloy 625. The 2020 table attaches “Grade 1” to the N06625 rows. If a quotation offers Alloy 625 flanges without naming the grade and the condition, ask which condition is being supplied before you compare prices.
  • If you are ordering a forged form in one of the three alloys whose forging entry became an ellipsis, confirm the product form with the supplier rather than assuming the 2003 table still applies.

How to specify a nickel alloy flange

The material specification and the grade go on the order line, and the dimensional standard goes with them. ASME SB-462 covers forged or rolled nickel alloy pipe flanges, forged fittings and valves for corrosive high-temperature service, and ASME SB-564 covers nickel alloy forgings. For the dimensions themselves, ASME B16.5 covers flanges up to NPS 24 and ASME B16.47 takes over from NPS 26 upward.

Our ASME B16.5-2003 flange dimensions page carries the Class 150, 300, 600 and 900 dimension tables with the corresponding nominal sizes and tolerances. For socket weld and threaded fitting dimensions, see our ASME B16.11 fitting dimensions reference, and for the boundaries between B16.9, B16.11 and MSS SP-43, our guide on which fitting standard applies to stainless fittings. For the size boundary between the two flange standards, see B16.5 or B16.47 at what size.

When you send an enquiry, state the nominal pipe size, the class, the flange type, the facing, the material specification with grade, and the dimensional standard you are working to. That last item is the one that determines whether a 2003 or a 2020 table is being applied.

Related reading

Frequently Asked Questions

What does “ASME B16.5-2020 vs 2003: What Changed for Nickel Alloy Flanges” cover?

The pressure-temperature numbers did not change. The material notes did, and they changed in a way that is easy to misread.