The most common specification mistake we see on zirconium enquiries is
ordering UNS R60705 where UNS R60702 was intended. R60705 is not a stronger
or better grade of zirconium: it is a niobium-bearing alloy, and its
chemistry, strength and corrosion behaviour differ enough that the two are
not interchangeable. Getting the grade right at the enquiry stage avoids a
lot of rework later.
ASME SB-658 covers three grades of seamless and welded zirconium pipe:
R60702, R60704 and R60705. The differences between them are worth setting out
before anything else is discussed.

| Element, wt pct | R60702 | R60704 | R60705 |
|---|---|---|---|
| Zirconium + hafnium, min | 99.2 | 97.5 | 95.5 |
| Hafnium, max | 4.5 | 4.5 | 4.5 |
| Iron + chromium | 0.2 max | 0.2 to 0.4 | 0.2 max |
| Tin | – | 1.0 to 2.0 | – |
| Niobium | – | – | 2.0 to 3.0 |
| Oxygen, max | 0.16 | 0.18 | 0.18 |
| Hydrogen, max | 0.005 | 0.005 | 0.005 |
| Nitrogen, max | 0.025 | 0.025 | 0.025 |
| Carbon, max | 0.05 | 0.05 | 0.05 |
| Tensile strength, min, ksi [MPa] | 55 [380] | 60 [415] | 80 [550] |
| Yield strength, min, ksi [MPa] | 30 [205] | – | – |
R60702 is the commercially pure grade and carries the strongest corrosion
resistance against hydrochloric and sulphuric acid. R60704 introduces 1 to
2 percent tin, which improves strength and is used where higher mechanical duty
is needed. R60705 introduces 2 to 3 percent niobium and reaches 80 ksi
[550 MPa] tensile, giving it the highest strength of the three with corrosion
resistance still ahead of most nickel alloys.


Zirconium is not a general corrosion resistant alloy. It has no useful
resistance to wet chlorine at elevated temperature, to oxidising acids
above about 65 degrees Celsius, or to alkalis at any concentration. If any
of those are present in the service, the material selection has to be
revisited rather than the grade adjusted.
| Product form | Specification | Grades |
|---|---|---|
| Seamless and welded pipe | ASME SB-658 / ASTM B658 | R60702, R60704, R60705 |
| Butt weld fittings | ASME SB-653 / ASTM B653 | R60702, R60704, R60705 |
| Forgings | ASME SB-493 / ASTM B493 | R60702 and higher grades |
| Tube | ASME SB-523 / ASTM B523 | R60702, R60704, R60705 |
| Bar and wire | ASME SB-550 / ASTM B550 | R60702 and higher grades |
| Strip, sheet and plate | ASME SB-551 / ASTM B551 | R60702 and higher grades |
Pipe is supplied to the nominal sizes and wall thicknesses of ASME B36.19M
for the S schedules, with outside diameter and wall tolerances to the tables
in SB-658. Thin wall pipe is treated separately for ovality, because thin
wall material develops significant out-of-roundness during final annealing
and straightening.
EN 10204 3.1 certification is issued per heat, quoting the grade, the
UNS number and the chemical analysis against SB-658 Table 1. Hydrostatic
testing is available and reported separately. Where the contract calls for
it, the material can be supplied with a specific reversible certificate and
third party inspection can be arranged at the works.
Zirconium is handled as a clean metal throughout. It is not carbon steel
with a coating, and a surface scratch or iron deposit becomes a corrosion
nucleus. We pack zirconium separately from steel and mark every bundle so the
receiving warehouse keeps it apart.
Please give the grade as the UNS number rather than the trade name, the
nominal size and schedule, the length, the quantity, and the certificate
requirement. If the enquiry is for a replacement of an existing line, the
existing material marking is usually sufficient for us to identify the
correct grade. If the service conditions are new to us, include the acid
concentration and temperature so we can confirm suitability before quoting.
Related items include our
zirconium butt weld fittings to ASME SB-653
and zirconium plate, sheet and bar,
which cover the same three grades in other product forms. For the wider
category see nickel alloy pipe and tube,
and the
acid service alloy selection
article covers where zirconium sits against the nickel alloys.
Zirconium pipe is proof tested to a rule of its own. ASME SB-658 clause 13.2 requires that each pipe 1/8 in. [3.2 mm] and larger in outside diameter, and with wall thickness of 0.015 in. [0.4 mm] and over, be tested to a hydrostatic pressure sufficient to produce a fiber stress of three fourths of the minimum yield strength of the pipe, provided that the test pressure does not exceed 5000 psi [35 MPa]. The pressure is calculated as P = 2St/D, where S is that three-fourths allowable fiber stress, t is the average wall thickness of the pipe and D is the nominal diameter.
That is a different rule from the one applied to nickel alloy seamless pipe under SB-829, and the difference is not cosmetic. SB-658 fixes the fiber stress as a fraction of the grade’s minimum yield strength rather than deriving an allowable from the material, it uses the average wall rather than the minimum permitted wall, and it caps the result instead of setting a floor.
The minimum yield strengths that feed the calculation are those of SB-658 Table 3: 30 ksi [205 MPa] for R60702, 35 ksi [240 MPa] for R60704 and 55 ksi [380 MPa] for R60705. Applying three fourths of each, the allowable fiber stress works out at 22 500 psi, 26 250 psi and 41 250 psi respectively. The table below gives the resulting maximum test pressure for each grade at each size and schedule, using the nominal wall thicknesses of SB-658 Table X1.1.
These pressures are our own calculation, worked out from the printed formula, the printed yield strengths and the printed nominal wall thicknesses. They are not values printed in the specification, and the actual test pressure on any given order is set by the mill against the pipe it has produced. Where the calculated figure exceeds the 5000 psi [35 MPa] limit of clause 13.2, the specification requires the lower pressure and the table says so.
The practical consequence is worth stating plainly. At the small sizes the calculated pressure runs above the 5000 psi [35 MPa] ceiling of clause 13.2, so the ceiling is what governs and the grade makes no difference to the test: at NPS 1/2 Schedule 40S all three grades are tested to 5 000 psi, because the calculated figures of 5 839, 6 812 and 10 705 psi all exceed it. The point at which the ceiling stops binding differs by grade, since R60705 carries 1.8 times the allowable fiber stress of R60702 (41 250 psi against 22 500 psi). For R60702 the calculated figure first falls below the ceiling at NPS 3/4 Schedule 40S, for R60704 at NPS 1-1/4 Schedule 40S, and for R60705 not until NPS 3-1/2 Schedule 40S. Below those points the grade does matter, because R60705 carries the higher fiber stress and is tested to a correspondingly higher pressure. At NPS 4 Schedule 40S, for example, R60702 is tested to 2 370 psi while R60705 is tested to 4 345 psi, and at NPS 12 Schedule 40S the three grades are tested to 1 324 psi, 1 544 psi and 2 426 psi.
SB-658 Table X1.1 is a reprint of Table 1 of ANSI B36.19 with SI units added, and it is the table to order against. Note one point of detail: at NPS 5 the specification prints an outside diameter of 5.583 in. [141.3 mm], while the ANSI B36.19 Table 1 reprints carried in SB-829, SB-775, SB-861 and SA-790 all print 5.563 in. [141.30 mm] for the same size. The two figures cannot both be right, since 5.583 in. converts to 141.8 mm, not 141.3 mm. We order and inspect to the mill’s certified dimension and flag the discrepancy rather than reconcile it ourselves.
Permissible diameter variations are given in SB-658 Table 4 for seamless pipe only: 1/64 in. [0.4 mm] over and 1/32 in. [0.8 mm] under up to NPS 1-1/2, widening to 3/32 in. [2.4 mm] over and 1/32 in. [0.8 mm] under from NPS 8 to NPS 12. Tolerances on welded pipe are as agreed between the manufacturer and the purchaser. Wall thickness variation is limited to 12.5 % of the nominal wall by clause 9.2, and for thin-wall pipe, defined as a wall of 3 % or less of the outside diameter, clause 9.1.2 limits ovality to 1.5 % of the specified outside diameter.
| NPS | Schedule | Nominal wall, in. (mm) | R60702 max test pressure | R60704 max test pressure | R60705 max test pressure |
|---|---|---|---|---|---|
| 1/8 | 40S | 0.068 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1/8 | 80S | 0.095 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1/4 | 40S | 0.088 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1/4 | 80S | 0.119 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 3/8 | 40S | 0.091 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 3/8 | 80S | 0.126 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1/2 | 40S | 0.109 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1/2 | 80S | 0.147 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 3/4 | 40S | 0.113 | 4,843 psi 33 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 3/4 | 80S | 0.154 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1 | 40S | 0.133 | 4,551 psi 31 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 1 | 80S | 0.179 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 11/4 | 40S | 0.140 | 3,795 psi 26 MPa | 4,428 psi 31 MPa | 5,000 psi (capped) 34 MPa |
| 11/4 | 80S | 0.191 | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 11/2 | 40S | 0.145 | 3,434 psi 24 MPa | 4,007 psi 28 MPa | 5,000 psi (capped) 34 MPa |
| 11/2 | 80S | 0.200 | 4,737 psi 33 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 2 | 40S | 0.154 | 2,918 psi 20 MPa | 3,404 psi 23 MPa | 5,000 psi (capped) 34 MPa |
| 2 | 80S | 0.218 | 4,131 psi 28 MPa | 4,819 psi 33 MPa | 5,000 psi (capped) 34 MPa |
| 21/2 | 40S | 0.203 | 3,177 psi 22 MPa | 3,707 psi 26 MPa | 5,000 psi (capped) 34 MPa |
| 21/2 | 80S | 0.276 | 4,320 psi 30 MPa | 5,000 psi (capped) 34 MPa | 5,000 psi (capped) 34 MPa |
| 3 | 40S | 0.216 | 2,777 psi 19 MPa | 3,240 psi 22 MPa | 5,000 psi (capped) 34 MPa |
| 3 | 80S | 0.300 | 3,857 psi 27 MPa | 4,500 psi 31 MPa | 5,000 psi (capped) 34 MPa |
| 31/2 | 40S | 0.226 | 2,542 psi 18 MPa | 2,966 psi 20 MPa | 4,661 psi 32 MPa |
| 31/2 | 80S | 0.318 | 3,578 psi 25 MPa | 4,174 psi 29 MPa | 5,000 psi (capped) 34 MPa |
| 4 | 40S | 0.237 | 2,370 psi 16 MPa | 2,765 psi 19 MPa | 4,345 psi 30 MPa |
| 4 | 80S | 0.337 | 3,370 psi 23 MPa | 3,932 psi 27 MPa | 5,000 psi (capped) 34 MPa |
| 5 | 40S | 0.258 | 2,080 psi 14 MPa | 2,426 psi 17 MPa | 3,812 psi 26 MPa |
| 5 | 80S | 0.375 | 3,023 psi 21 MPa | 3,526 psi 24 MPa | 5,000 psi (capped) 34 MPa |
| 6 | 40S | 0.280 | 1,902 psi 13 MPa | 2,219 psi 15 MPa | 3,487 psi 24 MPa |
| 6 | 80S | 0.432 | 2,934 psi 20 MPa | 3,423 psi 24 MPa | 5,000 psi (capped) 34 MPa |
| 8 | 40S | 0.322 | 1,680 psi 12 MPa | 1,960 psi 14 MPa | 3,080 psi 21 MPa |
| 8 | 80S | 0.500 | 2,609 psi 18 MPa | 3,043 psi 21 MPa | 4,783 psi 33 MPa |
| 10 | 40S | 0.365 | 1,528 psi 11 MPa | 1,783 psi 12 MPa | 2,801 psi 19 MPa |
| 10 | 80S | 0.500 | 2,093 psi 14 MPa | 2,442 psi 17 MPa | 3,837 psi 26 MPa |
| 12 | 40S | 0.375 | 1,324 psi 9 MPa | 1,544 psi 11 MPa | 2,426 psi 17 MPa |
| 12 | 80S | 0.500 | 1,765 psi 12 MPa | 2,059 psi 14 MPa | 3,235 psi 22 MPa |
Related reading: zirconium pipe schedule and wall thickness table, zirconium forging fittings in SB-653 and nickel alloy pipe and tube product range.