A nickel alloy flange order usually carries two numbers, and buyers who
expect one specification to answer both questions end up with a non-conforming
part. One number says where the geometry comes from — ASME B16.5 for
flanges up to NPS 24, ASME B16.47 above that, ASME B16.9 for butt-weld
fittings and ASME B16.11 for socket-weld and threaded fittings. The other says
where the material comes from. For corrosion-resistant nickel alloys there are
three candidate material specifications, and they are not interchangeable:
SB-462 for forged flanges and forged fittings, SB-366 for factory-made
wrought welding fittings, and SB-564 for nickel alloy forgings generally. This
guide sets out which one governs which product form, and what the SB-462
specification actually requires once you have selected it.
Everything below is taken from ASME BPVC Section II Part B, and the grade
list is checked against the scope clause rather than a supplier brochure. That
matters more than it sounds: the SB-462 grade list has changed between
editions, and a purchase order written against an old specification can name
a grade that the current one no longer covers.
| Material specification | Product form it governs | Dimensional standard | Grades it covers |
|---|---|---|---|
| ASME SB-462 | Forged or rolled pipe flanges, forged fittings, valves and parts for corrosive high-temperature service | ASME B16.5 (NPS 1/2 to 24), ASME B16.47 (NPS 26 and above) | 18 UNS designations listed in clause 1.1 |
| ASME SB-366 / SB-366M | Factory-made wrought welding fittings: butt-weld to B16.9 and socket-weld and threaded to B16.11. Does not apply to cast fittings | ASME B16.9, B16.11, MSS SP-43, SP-95, SP-97 | A separate and much longer grade list, including UNS N06625 and UNS N04400, which SB-462 does not cover |
| ASME SB-564 | Nickel alloy forgings — the general forging material specification, and the parent specification from which many forged fittings and flanges are made | As specified on the forging sketch or drawing | 37 UNS designations, including UNS N06625, UNS N04400 and UNS N06044, none of which are in the SB-462 list |
The three overlap in practice, and the boundary is where ordering errors
come from. A Hastelloy C-276 weld neck flange is an SB-462 product: C-276
(UNS N10276) is one of the eighteen grades SB-462 names, and SB-462 is the
specification written for forged flanges in corrosive high-temperature service.
An Inconel 625 forged flange is not an SB-462 product at all — UNS
N06625 does not appear in the SB-462 scope clause — so it is made to
SB-564 and dimensioned to B16.5. The same is true of Monel 400 (UNS N04400)
forgings. The material specification and the dimensional standard have to be
named separately on the purchase order, and they do not come from the same
family of documents.
SB-462 Table 2 gives the room-temperature mechanical property minimums for
each covered grade. Every value below is taken from that table. Note that
ASME prints the SI values in parentheses as mathematical conversions provided
for information only, so the two systems are not exact equivalents; the inch-pound
value is the standard one.
| Grade | Common designation | Tensile strength, min | Yield strength, 0.2% offset, min | Elongation in 2 in. or 50 mm, min, % | Reduction of area, min, % |
|---|---|---|---|---|---|
| UNS N06030 | Alloy 30 (Ni-Cr-Fe-Mo-Cu) | 85 ksi (586 MPa) | 35 ksi (241 MPa) | 30 | not specified |
| UNS N06035 | Alloy 35 (low-carbon Ni-Cr-Mo) | 85 ksi (586 MPa) | 35 ksi (241 MPa) | 30 | not specified |
| UNS N06022 | Hastelloy C-22 | 100 ksi (690 MPa) | 45 ksi (310 MPa) | 45 | not specified |
| UNS N06200 | Alloy 2000 | 100 ksi (690 MPa) | 45 ksi (310 MPa) | 45 | not specified |
| UNS N06059 | Alloy 59 (low-carbon Ni-Cr-Mo) | 100 ksi (690 MPa) | 45 ksi (310 MPa) | 45 | not specified |
| UNS N10362 | Alloy 36 (low-carbon Ni-Cr-Mo) | 105 ksi (725 MPa) | 45 ksi (310 MPa) | 40 | not specified |
| UNS N06686 | Alloy 686 (low-carbon Ni-Cr-Mo-W) | 100 ksi (690 MPa) | 45 ksi (310 MPa) | 45 | not specified |
| UNS N08020 | Alloy 20 (Ni-Cr-Fe-Mo-Cu) | 80 ksi (551 MPa) | 35 ksi (241 MPa) | 30 | 50 |
| UNS N08367 | Alloy 367 (Ni-Cr-Mo-Fe-N) | 95 ksi (655 MPa) | 45 ksi (310 MPa) | 30 | 50 |
| UNS N10276 | Hastelloy C-276 | 100 ksi (690 MPa) | 41 ksi (283 MPa) | 40 | not specified |
| UNS N10665 | Alloy B-2 (Ni-Mo) | 110 ksi (760 MPa) | 51 ksi (350 MPa) | 40 | not specified |
| UNS N10675 | Alloy B-3 (Ni-Mo) | 110 ksi (760 MPa) | 51 ksi (350 MPa) | 40 | not specified |
| UNS N10629 | Alloy B-10 (Ni-Mo) | 110 ksi (760 MPa) | 51 ksi (350 MPa) | 40 | not specified |
| UNS N08031 | Alloy 31 (low-carbon Ni-Fe-Cr-Mo-Cu) | 94 ksi (650 MPa) | 40 ksi (276 MPa) | 40 | not specified |
| UNS N06045 | Alloy 45 (Ni-Cr-Fe-Si) | 90 ksi (620 MPa) | 35 ksi (241 MPa) | 35 | not specified |
| UNS N06025 | Alloy 25 (Ni-Cr-Fe-Al) | 98 ksi (680 MPa) | 39 ksi (270 MPa) | 30 | not specified |
| UNS N06699 | Alloy 699 (Ni-Cr-Fe-Mo-N) | 89 ksi (610 MPa) | 35 ksi (240 MPa) | 40 | not specified |
| UNS R20033 | Alloy 33 (Cr-Ni-Fe-N) | 109 ksi (750 MPa) | 55 ksi (380 MPa) | 40 | not specified |
Two grades carry a specified reduction of area and sixteen do not. Where
SB-462 prints no value, the requirement is the elongation figure alone. The
yield strength values are the ones to watch on a purchase order: UNS N10276
(C-276) is specified at 41 ksi (283 MPa) while UNS N06022 (C-22) and UNS
N06200 (Alloy 2000) are both specified at 45 ksi (310 MPa), despite the three
grades having the same 100 ksi (690 MPa) tensile minimum. A buyer who
substitutes one grade for another on the strength of the tensile figure alone
will pick up a lower yield than the specification requires.
SB-462 clause 5.3 sets the delivery condition by grade, and NOTE 2 gives
the recommended annealing temperature range for each one, all followed by water
quenching or rapid cooling by other means. This table is the single most
useful document in the specification for a buyer, because the annealing
temperature differs grade by grade — there is no single figure you can
write on the order and be safe for every alloy.
| Grade | Delivery condition | Recommended annealing temperature | Cooling method |
|---|---|---|---|
| UNS N06030 | solution annealed | 2125–2175 °F (1163–1191 °C) | Water quench or rapid cooling |
| UNS N06035 | solution annealed | 2025–2075 °F (1107–1135 °C) | Water quench or rapid cooling |
| UNS N06022 | solution annealed | 2025–2075 °F (1107–1135 °C) | Water quench or rapid cooling |
| UNS N06200 | solution annealed | 2075–2125 °F (1135–1163 °C) | Water quench or rapid cooling |
| UNS N06059 | solution annealed | 2025–2125 °F (1107–1163 °C) | Water quench or rapid cooling |
| UNS N10362 | solution annealed | 2075–2125 °F (1135–1163 °C) | Water quench or rapid cooling |
| UNS N06686 | solution annealed | 2125–2225 °F (1163–1218 °C) | Water quench or rapid cooling |
| UNS N08020 | stabilized annealed | 1700–1850 °F (927–1010 °C) | Water quench or rapid cooling |
| UNS N08367 | solution annealed | 5.3.2.1 minimum 2025 F (1105 C), quench in water | Water quench or rapid cooling |
| UNS N10276 | solution annealed | 2025–2075 °F (1107–1135 °C) | Water quench or rapid cooling |
| UNS N10665 | solution annealed | 1925–2000 °F (1052–1093 °C) | Water quench or rapid cooling |
| UNS N10675 | solution annealed | 1925–2000 °F (1052–1093 °C) | Water quench or rapid cooling |
| UNS N10629 | solution annealed | 1925–2000 °F (1052–1093 °C) | Water quench or rapid cooling |
| UNS N08031 | solution annealed | 2050–2160 °F (1121–1182 °C) | Water quench or rapid cooling |
| UNS N06045 | solution annealed | 2125–2190 °F (1163–1199 °C) | Water quench or rapid cooling |
| UNS N06025 | solution annealed | 2175–2240 °F (1191–1227 °C) | Water quench or rapid cooling |
| UNS N06699 | solution annealed | 1975–2065 °F (1080–1130 °C) | Water quench or rapid cooling |
| UNS R20033 | solution annealed | 2010–2150 °F (1100–1180 °C) | Water quench or rapid cooling |
UNS N08020 (Alloy 20) is the exception that proves the rule: it is
furnished in the stabilized-annealed condition at 1700 to 1850 degrees F (927
to 1010 degrees C), which is a lower and completely different thermal cycle
from the solution anneal the corrosion-resistant grades receive. UNS N08367
(Alloy 367) has its own rule in clause 5.3.2.1: heating to a minimum of
2025 degrees F (1105 degrees C) followed by a water quench. Heat treatment may
be performed before machining, so the mill certificate records the cycle
applied to the billet, not to the finished flange face.
SB-462 clause 7.2 is more precise than most buyers assume, and the three
sub-clauses distinguish three different situations that are routinely
conflated.
| Clause | Requirement | What it means on the order |
|---|---|---|
| 7.2 | After machining, valve bodies, fittings and other pressure-containing parts shall be tested to the hydrostatic shell-test pressures prescribed in ANSI B16.5 for the applicable alloy steel rating for which the forging is designed, and shall show no leaks | A forged fitting or valve body is pressure-tested. The test pressure is the B16.5 shell test for the rating, not a number you choose |
| 7.2.1 | No hydrostatic test is required for welding neck or other flanges | A weld neck flange is not individually shell-tested. If the purchase order requires a flange test, it has to say so — the specification does not oblige the mill to do it |
| 7.2.2 | The forging manufacturer is not required to pressure-test rough forgings that are to be finally machined by others, and the fabricator of finished parts is not required to pressure-test forgings that are designed to be pressure-containing only after assembly by welding into a larger structure | The obligation transfers with the work. The forging manufacturer remains responsible under clause 15.1 for the performance of the forging under the final test |
| 7.3 | Macroetch tests shall show sound and reasonably uniform material. If, on successive tests, 10% of any heat fails the macroetch requirement, all forgings from that heat shall be rejected | The 10% figure is a rejection trigger for the whole heat, not a sample-acceptance allowance |
Two of these catch buyers out. The first is that a weld neck flange is not
hydrostatically tested as a matter of course, while a forged elbow is. If a
project specification requires every pressure-containing component to be
shell-tested, that requirement has to reach the flange explicitly. The second
is the macroetch rule: it is easy to read 10% as a permissible failure rate
for the heat, and it is the opposite. Once 10% of a heat fails, the whole
heat is rejected.
SB-462 carries the note that it is identical with ASTM Specification
B462-18 except that certification and a test report have been made
mandatory. That single sentence is the whole practical difference between the
two document sets, and it is worth putting on the order. SB-564 carries the
same kind of note against ASTM B564-17a, and SB-366 states that its listed
heat treatments are mandatory where ASTM leaves them optional.
| Specification | ASTM equivalent | What ASME changes |
|---|---|---|
| ASME SB-462 | ASTM B462-18 | Certification and a test report are mandatory. The specification text itself marks the required content: the material shall be manufactured, sampled, tested and inspected in accordance with the specification, and a report of the test results shall be furnished |
| ASME SB-564 | ASTM B564-17a | Certification and test reports are made mandatory, along with further provisions |
| ASME SB-366 / SB-366M | ASTM B366/B366M-17 | The listed heat treatments are mandatory in clause 5.3 |
Under ASTM B462 the certification clause is conditional — the
producer’s or supplier’s certification is furnished when the purchaser
specifies it in the order or contract. Under ASME SB-462 it is not
conditional. An order that says only “ASTM B462” and an order that says
“ASME SB-462” therefore ask for different amounts of documentation, and the
difference is invisible until the documents arrive with the shipment. Product
marking follows MSS SP-25 and must carry the manufacturer’s symbol or name,
the designation of service rating, the specification, the grade of material
and the size.
Clause 4.1 lists what the purchaser has to specify, and the list is short
enough to copy onto an enquiry. It covers quantity by weight or number of
pieces, the name of material or the UNS number, the forging sketch where
required, forging sectioning where required, the ASTM designation and year of
issue, inspection, any supplementary requirements, and if possible the
intended end use. The specification gives a worked example of a typical
ordering description: 200 forgings, UNS N08020, in accordance with the
attached drawing and Specification B462.
Two supplementary requirements are worth knowing about. S1 applies to
UNS N08020 and requires one intergranular corrosion test per heat on a
sensitized specimen, tested in accordance with Practices A262, with the
specific practice named on the order — if Practice B is specified, the
specimen must pass with a rate below 0.002 inches per month. S2 requires
positive material identification on 100% of the product by Guide E1916, and
all product that is not of the correct material grade shall be rejected.
Both apply only when the purchaser names them, which is precisely why they
have to be named.
For the dimensional half of the order, the flange dimensions for Class 150,
300, 600 and 900 across NPS 1/2 to NPS 24 are set out in our
the Class 150 to 900 flange dimensions,
and the boundary between B16.5 and B16.47 is explained in
where B16.5 stops and B16.47 begins.
If the material is UNS N10276 or UNS N06022 rather than UNS N06625, the
flange is covered by
the C-276, C-22 and Alloy 2000 forged flange page;
the grades on the opposite side of the forging boundary are in
the Alloy 699, 59, 686 and 30 SB-462 page,
and the UNS N06625 forged fittings are in
the Inconel 625 butt-weld fitting range. For the matching pipe and tube
materials, see the round pipe we hold in stock.
No. UNS N06625 does not appear in the SB-462 scope clause. An Inconel 625
forged flange or fitting is made to ASME SB-564 and dimensioned to ASME B16.5
or B16.47. A 625 butt-weld fitting to B16.9 is made to ASME SB-366. Both
documents exist and both are frequently quoted by suppliers as though SB-462
were a third option for 625, which it is not.
UNS N04400 is not an SB-462 grade either. Monel 400 forgings fall under
ASME SB-564, and wrought Monel 400 fittings under SB-366. The dimensional
standard is still ASME B16.5 or B16.47 for a flange.
Not under the default requirements of SB-462. Clause 7.2.1 states that no
hydrostatic test is required for welding neck or other flanges. Forged
fittings and valve bodies are tested to the B16.5 shell-test pressure under
clause 7.2. If your project specification requires flange testing, state it
on the order.
Not by default. The ASTM B462 certification clause is conditional on the
purchaser specifying it in the order or contract. ASME SB-462 makes
certification and a test report mandatory, which is the substantive
difference between the two document sets.
Eighteen, as listed in clause 1.1 of the current edition. The list has
changed between editions: the earlier ASTM B462-06 list included UNS N08024
and UNS N08026 and did not include UNS N10362 or UNS N06699, so an order
copied from an old specification may name a grade the current specification
does not cover. Write the grade and the year of the specification you want
on the order.
No. Clause 5.3 sets the delivery condition by grade, and the ASME edition
makes those heat treatments mandatory, so a product ordered to SB-462 is
supplied in the specified condition. What you should check on the certificate
is that the annealing temperature recorded falls inside the range for your
grade.