A purchase order for forged fittings and flanges is written months before the parts arrive. Between the two sits a document most buyers never read closely: SA-961, the general requirements specification for forged fittings, valves and flanges. It decides what the mill must prove, what it must mark on the part, and what it may do to a part that fails a test.
This is a checklist of the points at which a fitting is accepted or rejected.
Bolting is the part of a flanged joint that most often arrives as a copy rather than a calculation, and it has its own two specifications. SA-193 covers the studs, SA-194 covers the nuts, and SA-962 holds the common requirements both inherit.
The first thing to establish is that a stud grade and a nut grade are not interchangeable, and that the specification will not let the mill substitute one for the other. SA-194 clause 1.1 states it in a single sentence: grade substitutions without the purchaser’s permission are not allowed.
SA-194 clause 1.1 covers nuts in the size range 1/4 through 4 in. and metric M12 through M100 nominal, with austenitic stainless steel nuts from 1/4 in. and M12 nominal up. SA-193 clause 1.1 covers alloy and stainless steel bolting materials for pressure vessels, valves, flanges and fittings, and points to SA-962 for the definition of bolting.
Then there is the hardness question, and it is where bolting specifications earn their reputation. SA-193 Table 2 sets the austenitic grades in their solution-treated condition, and SA-194 Table 2 bounds the nuts.
| Component | Grade | Size band | Tensile / yield, ksi | Hardness ceiling |
|---|---|---|---|---|
| Stud, SA-193 | B7 chromium-molybdenum | to 2.5 in. | 125 / 105 | 321 HBW, or 35 HRC |
| Stud, SA-193 | B7 chromium-molybdenum | over 4 to 7 in. | 100 / 75 | 321 HBW, or 35 HRC |
| Stud, SA-193 | B7MA chromium-molybdenum | to 4 in. | 100 / 80 | 235 HBW, or 99 HRB |
| Stud, SA-193 | B8 Class 1 and 1D, austenitic | all diameters | 75 / 30 | 223 HBW, or 96 HRB |
| Stud, SA-193 | B8 Class 1A, austenitic | all diameters | 75 / 30 | 192 HBW, or 90 HRB |
| Nut, SA-194 | 2H | to 1.5 in. or M36 | not stated | 248-327 HBW with 24-35 HRC |
| Nut, SA-194 | 8, 8C, 8CLN, 300-series | not stated | not stated | 126-300 HBW, 32 HRC max |
| Nut, SA-194 | 8A, 8CA, 8CLNA, Class 1A | not stated | not stated | 126-192 HBW with 60-90 HRB |
Two details earn a second look. B7 in the smaller diameter band carries 125 ksi tensile and 105 ksi yield, while the same grade over 4 to 7 in. drops to 100 ksi and 75 ksi — the strength floor falls with diameter. And B7MA, at the same size, carries 235 HBW or 99 HRB against B7’s 321 HBW or 35 HRC.
Austenitic Class 1 and Class 1A studs are not the same part. Class 1A is carbide solution treated in the finished condition and carries 192 HBW or 90 HRB against Class 1’s 223 HBW or 96 HRB, with the same 75 ksi tensile and 30 ksi yield in both. Where a joint must stay below a hardness ceiling, that is the decision.
SA-961 clause 16 governs weld repair, and it starts with who decides. Clause 16.1 states that the purchaser may require proposed weld repairs to be submitted for approval by invoking the appropriate supplementary requirement in the purchase order. If the purchaser does not require prior approval, these repairs shall be permitted at the supplier’s discretion. Without it, the mill decides whether to repair a defect and does not have to ask.
The repair itself is tightly bounded. Clause 16.1.1 requires the welding procedure and welders to be qualified in accordance with Section IX of the ASME Boiler and Pressure Vessel Code. Clause 16.1.2 requires defects to be completely removed prior to welding by chipping or grinding to sound metal, verified by magnetic particle inspection per A275/A275M or Guide E709 for ferritic, martensitic or ferritic-austenitic grades, or liquid penetrant inspection per E165/E165M for austenitic grades. Clause 16.1.3 requires the welded area ground smooth to the original contour and completely free of defects.
Clause 14.1 covers a failed test specimen. When representative or retest specimens do not conform to the product specification for the tested characteristic, the product may be reworked: clause 14.1.1 permits rework by heat treatment and retest if previously tested unheat treated, and clause 14.1.2 permits reheat treatment and retest if previously tested heat treated.
SA-961 clause 20.1 lists the marking requirements: product specification number, grade or marking symbol, class, certifying organization’s name or symbol, heat number, size, and service rating if applicable, marked legibly and in a position that does not injure the forging. The class letter is the one people miss. SA-403 clause 5.3 names six dimensional standards for a Class S fitting without saying which governs dimensions, so the order must select one.
On certification, SA-961 clause 19.1 requires both a test report and a certificate of compliance. Clause 19.2 requires the test report to carry the product specification number and year/date of issue, the results of all tests required by the specification and the purchaser order, and to be traceable to the part represented; clause 19.3 allows one document to carry both. Clause 19.5 carries the responsibility: notwithstanding the absence of a signature, the organization submitting the certificate is responsible for its content.
SA-961 clause 18 covers rejection: clause 18.1 requires samples representing rejected material to be preserved until disposition has been agreed between manufacturer and purchaser, and clause 18.2 states that material showing injurious defects after acceptance at the manufacturer’s works will be rejected, with the manufacturer notified.
One supplementary requirement is worth calling out separately because it is the one most often left off an order. SA-961 Supplementary Requirement S60 is the positive material identification requirement. S60.1 states that forgings shall receive positive material identification to ensure the purchaser is receiving forgings of the correct material grade prior to shipment. S60.2 requires the examination per Guide E1916, S60.3 requires 100 % of the forgings to be examined, and S60.4 requires all off-grade forgings to be rejected.
The nickel alloy flanges and fittings have their own counterpart. SB-462, covering forged or rolled nickel alloy pipe flanges, forged fittings and valves, carries Supplementary Requirement S1 for corrosion tests on UNS N08020 and S2 for positive material identification. S1.1 requires one intergranular corrosion test per heat on a sensitised specimen tested per Practices A262, with the practice, B or E, specified on the order; if Practice B is specified, the specimen must pass below 0.002 inches per month.
SB-462 clause 1.1 covers UNS N06030, N06035, N06022, N06200, N06059, N10362, N06686, N08020, N08367, N10276, N10665, N10675, N10629, N08031, N06045, N06025, N06699 and R20033 in pipe flanges, forged fittings and valves for corrosive high-temperature service. Check the alloy against that list first.
| Checkpoint | Clause | What to confirm |
|---|---|---|
| Nut grade on the order | SA-194 §1.1 | No substitution without the purchaser’s permission |
| Stud hardness band | SA-193 Table 2 | B7 321 HBW/35 HRC; B7MA 235 HBW/99 HRB; B8 Cl.1 223 HBW/96 HRB |
| Nut hardness band | SA-194 Table 2 | 8-series 126-300 HBW, 32 HRC max; 8A 126-192 HBW |
| Weld repair approval | SA-961 §16.1 | Invoke to require prior approval of weld repairs |
| Marking content | SA-961 §20.1 | Spec number, grade, class, certifying organisation, heat number, size |
| Dimensional standard named | SA-403 §5.3 | Class S: name one of B16.9, B16.11, MSS SP-79/83/95/97 |
| PMI on forgings | SA-961 S60.2 to S60.4 | Guide E1916, 100 % of forgings, off-grade rejected |
| PMI on nickel alloy product | SB-462 S2.3, S2.4 | 100 % examined, off-grade rejected |
| Alloy 20 corrosion test | SB-462 S1.1 | One intergranular test per heat, sensitised 1 h |
| Test report and certificate | SA-961 §19.1 to §19.3 | Both required; one combined document permitted |
| Certificate responsibility | SA-961 §19.5, SA-999 §25.1 | Submitting organisation is responsible for content |
| Hydrostatic test invoked | SA-961 §13.1 | Performed only when the purchaser invokes it |
That last row is the one to look at twice. SA-961 clause 13.1 states that parts shall be capable of passing a hydrostatic test compatible with the rating of the finished part, and that such tests shall be conducted by the supplier only when the purchaser invokes the hydrostatic test supplementary requirement. The capability is guaranteed. The test is yours to ask for.
Send us the alloy, the fitting or flange type, the size range and the service conditions, and we will return a written material proposal naming the grade symbol, the class and the supplementary requirements that apply. Message our export desk on WhatsApp, or start from the our forged fitting range and the forged fittings category to see what is available, then use the our export enquiry form to request a quote.
A purchase order for forged fittings and flanges is written months before the parts arrive. Between the two sits a document most buyers never read closely: SA-961, the general requirements specification for forged fittings, valves and flanges.
Need certified material with traceable test reports? Request a quote from Tailan Metal and our team will confirm grade, specification and certification for your service condition.