Impact Testing and Certification for Nickel Alloy Fittings

SA-961 routes impact requirements to the product specification and to supplementary requirements, so a fitting order that is silent on impact testing has not chosen whether the part is tested. This is what the clauses require and what the purchaser has to state.

A fitting order that says nothing about impact testing has not chosen whether the part is impact tested. The fittings specification does not set the requirement itself. It routes the requirement to the product specification, and it adds the supplementary requirements that turn a routine order into a tested one. For nickel alloy flanges and forgings supplied into European pressure equipment work, that routing is where the money and the paperwork sit.

What SA-961 Section 12 actually requires

SA-961 is the general requirements specification for forged fittings, valves and flanges. Its Section 12 carries the impact requirements, and the clauses read as a short chain of decisions rather than as a single obligation.

ClauseRequirementWhat the purchaser has to supply
§12.1The part shall conform to the impact requirements prescribed in the product specificationWhich product specification applies, and whether impact testing is invoked at all
§12.2Sampling for impact testing shall conform to the product specificationNothing separately; the product specification controls the sample count
§12.3Simple-beam Charpy type A with a V-notch, to ASTM A370, or A1058 where the M suffix SI track is specified. Standard specimens 10 by 10 mm are used unless the material is too thin, in which case the largest obtainable standard subsize is usedThe unit system, because it selects the test method document
§12.3, final sentenceWhere the finished part is too small to permit the smallest standard subsize specimen, an impact test by the part manufacturer is not requiredNothing, but note it: a small part can lawfully arrive with no impact test at the fitting stage
§12.4A retest is permitted where the average meets the requirement but one specimen falls below the individual minimum: two specimens adjacent to and on either side of the failed one, each meeting the minimum averageNothing
S54.1Three Charpy V-notch impact energy specimens from a representative forging of each heat, at a location agreed between the certifying organisation and the purchaserAgreement on the specimen location, in advance
S54.2The purchaser shall supply the impact test temperature and the required minimum requirements for the test, including the lowest single absorbed energy for a single specimen where an average absorbed energy is requiredThe test temperature and the acceptance values. This cannot be defaulted by the mill
S63.1 to S63.5Pressure equipment directive mechanical testing: Charpy at the lowest scheduled operating temperature but not above 68 F (20 C); the same frequency as the tension test, with three individual Charpy specimens per required tension test; minimum impact absorption energy 20 ft/lb (27 J); minimum elongation 14 percent on a gauge length of five times the test specimen diameter; results included in the product certificationConfirmation that the supplementary requirement is invoked, and the scheduled operating temperature

Two practical points fall out of that table. First, S54.2 puts the test temperature in the purchaser’s hands. A supplier cannot supply it, and a mill that quotes impact testing without a stated temperature has quoted an incomplete test. Second, the PED requirement in S63 is anchored to the lowest scheduled operating temperature of the finished equipment, capped at 68 F (20 C), so a 300 F service does not imply a 300 F Charpy test. The scheduled operating temperature is the input that decides the test, and it is the buyer’s input to declare.

For forgings, the temperature is fixed and the energy is not

Where the product specification is SA-182 for a forging, the impact test temperature is already determined: SA-182 Section 9.7.5 sets it at 0 F (-18 C), with Section 9.7.4 requiring a minimum average energy absorption of 40 ft-lbf (54 J) for three specimens and allowing one specimen in a set below that average provided it still meets 35 ft-lbf (48 J). Subsize specimens for material limitations need prior purchaser approval. So for a forged nickel alloy flange the discussion is about whether impact testing is invoked and how the forgings are sampled, not about where the temperature comes from.

The other requirement that a purchaser should look for on a forging is the marking. SA-182 Section 19.1.2 requires forgings repaired by welding to carry the letter W after the specification designation, and where a repair-welded austenitic stainless forging has not been post-weld heat treated in accordance with Table 4, the letters WNS. A fitting order that receives weld-repaired forgings without naming the marking position leaves the acceptance decision open at receipt rather than at the order.

The stud and the nut are not one specification

Bolting on a nickel alloy flange package is specified separately from the flange itself, and the hardness limits on studs and nuts are set in different documents. The pairing that matters most in corrosive service is the austenitic bolting, where the stud grade and the nut class each have their own hardness ceiling.

ComponentGradeMinimum tensile / yield, ksiMaximum hardness
Stud (SA-193)B7, chromium molybdenum, 2.5 percent and under125 / 105321 HBW or 35 HRC
Stud (SA-193)B7MA, chromium molybdenum, 4 percent and under100 / 80235 HBW or 99 HRB
Stud (SA-193)B8, Classes 1 and 1D, austenitic, carbide solution treated75 / 30223 HBW or 96 HRB
Stud (SA-193)B8, Class 1A, austenitic, carbide solution treated in the finished condition75 / 30192 HBW or 90 HRB
Nut (SA-194)Class 8 and 8C family, austeniticStrength by size126 to 300 HBW, 32 HRC max, 60 HRB min
Nut (SA-194)Class 8A family, austeniticStrength by size126 to 192 HBW, 60 to 90 HRB
Nut (SA-194)2H heavy hex, to 1-1/2 in. (M36) incl.Strength by size248 to 327 HBW, 24 to 35 HRC
Nut (SA-194)2H heavy hex, over 1-1/2 in. (M36)Strength by size212 to 327 HBW, 35 HRC max

The practical consequence is that a stud grade and a nut class have to be specified as a pair. The Class 8A nut family is the softer austenitic option, with a 192 HBW or 90 HRB ceiling, and pairing it with a B8 Class 1 stud at 223 HBW or 96 HRB produces an assembly whose two halves have deliberately different hardness limits. That is sometimes what a client wants and sometimes not, and it cannot be achieved by accident.

The rest of the acceptance package

  • Hydrostatic test. SA-961 Section 13.1 requires parts to be capable of passing a hydrostatic test compatible with the rating of the finished part, but states that such tests are conducted by the supplier only when the hydrostatic test supplementary requirement in the product specification is invoked by the purchaser. An order that does not invoke it gets no hydrostatic test from the fitting maker.
  • Positive material identification. SA-961 S60 requires PMI to ASTM E1916 on 100 percent of the forgings before shipment, so that no grade mix-up occurs during manufacturing and marking; all product not of the correct grade shall be rejected, and the marking method after examination shall be agreed between manufacturer and purchaser.
  • Test report and certificate of compliance. SA-961 Section 19.1 requires both, and Section 19.2 requires the test report to carry the product specification number and year and date of issue, the results of all tests required, and the purchaser order, and to be traceable to the part represented. Traceability to the individual part is the clause worth holding a supplier to.
  • Hardness. SA-182 Section 9.6.1 requires a minimum of two pieces per batch or continuous run to be hardness tested to the limits in Table 3, and permits the purchaser to verify by testing at any location on the forging provided the testing does not render the forging useless.
  • Repair welding. SA-961 Section 16.1.4 caps repair welding at 10 percent of the surface area of the part, or 33-1/3 percent of the wall thickness of the finished product, or 3/8 in. (10 mm) deep at the location of the repair, and Section 16.1.1 requires the welding procedure and welders to be qualified to Section IX of the ASME Code.
  • The certificate itself. SA-999 Section 25.1 requires a certificate of compliance stating that the product was manufactured, sampled, tested and inspected in accordance with the specification, including year-date, the supplementary requirements and any other requirements designated in the purchase order, and states that a signature or notarization is not required provided the document is dated and identifies the submitting organisation. Section 25.1.1 keeps that organisation responsible for the content regardless.

We supply our stainless steel pipe fittings and the forged flange product pages, and the bolting to match on our nickel alloy bolting range. We can supply the parts with the impact, PMI, hydrostatic and certification requirements your contract names, documented to the clause. If you want a package quoted against a specific set of supplementary requirements, request a fitting and flange quote and send us the clauses you need invoked, the scheduled operating temperature, and whether weld-repaired forgings are acceptable to you.

Frequently Asked Questions

What does “Impact Testing and Certification for Nickel Alloy Fittings” cover?

A fitting order that says nothing about impact testing has not chosen whether the part is impact tested. The fittings specification does not set the requirement itself.

Related Products

Need certified material with traceable test reports? Request a quote from Tailan Metal and our team will confirm grade, specification and certification for your service condition.

These test and certification obligations attach to the fitting forms listed in our nickel alloy butt weld and socket weld fittings guide.

Product Enquiry