ASME SB-162 is the specification for rolled nickel plate, sheet and strip,
and it covers exactly two UNS designations: N02200 and N02201. That is worth
stating up front, because the commercially pure nickel family is broader than
the plate standard alone and buyers regularly arrive with a rod or bar
enquiry against a plate enquiry, expecting the same material.
The three commercially pure nickel grades in ASME Section II are Nickel 200
(N02200), Nickel 201 (N02201) and solution-strengthened Nickel N02211.
SB-160 covers N02200 and N02201 in rod and bar form, and adds N02211.
SB-162 covers N02200 and N02201 in plate, sheet and strip. The mechanical
requirements differ between them, and the chemical requirements differ
between N02200 and N02201 on carbon alone.

| Element, wt pct | Nickel 200 (N02200) | Nickel 201 (N02201) |
|---|---|---|
| Nickel, min | 99.0 | 99.0 |
| Copper, max | 0.25 | 0.25 |
| Iron, max | 0.40 | 0.40 |
| Manganese, max | 0.35 | 0.35 |
| Carbon, max | 0.15 | 0.02 |
| Silicon, max | 0.35 | 0.35 |
| Sulfur, max | 0.01 | 0.01 |
Every other element is identical. The grades differ in carbon and nothing
else, which is why the choice is a service decision rather than a property
decision: Nickel 201 with its 0.02 percent carbon maximum is preferred in
caustic service, because carbon in caustic is what picks up intergranular
attack, while Nickel 200 with its 0.15 percent maximum is the grade used
where the material is cold worked rather than hot formed.
| Condition | Tensile strength, min, psi [MPa] | Yield strength, min, psi [MPa] | Elongation in 2 in., min, pct |
|---|---|---|---|
| N02200 hot-rolled plate, annealed | 55 000 [380] | 15 000 [100] | 40 |
| N02200 hot-rolled plate, as-rolled | 55 000 [380] | 20 000 [135] | 30 |
| N02200 hot-rolled sheet, annealed | 55 000 [380] | 15 000 [100] | 40 |
| N02200 cold-rolled sheet, annealed | 55 000 [380] | 15 000 [100] | 40 |
| N02200 cold-rolled sheet, hard | 90 000 [620] | 70 000 [480] | 2 |
| N02201 hot-rolled plate, annealed | 50 000 [345] | 12 000 [80] | 40 |
| N02201 hot-rolled plate, as-rolled | 50 000 [345] | 12 000 [80] | 30 |
| N02201 cold-rolled sheet and strip, annealed | 50 000 [345] | 12 000 [80] | 40 |
Yield strength requirements do not apply to material under 0.020 inch
thickness, and Rockwell hardness conversions should be treated with care on
material under 0.050 inch. Both points matter when the enquiry is for a thin
foil or a precision shim rather than a vessel wall.


EN 10204 3.1 certification is issued per heat with the chemical analysis
against SB-162 Table 2 and the condition actually supplied, quoted as
annealed, as-rolled or a cold-worked temper. Where the enquiry is for sheet
in a defined temper, the hardness range from SB-162 Table 3 is stated on the
certificate. Thickness, width and length are certified against the
dimensional tables of the specification.
Commercially pure nickel is a soft, easily worked material and it is
supplied with a protective surface film or paper interleave. That protection
is part of the specification intent, not an extra, and we do not ship nickel
plate bare unless the order asks for it.
State the grade as Nickel 200 or Nickel 201, the form (plate, sheet or
strip), the thickness, the width and length, the condition, and the quantity.
If the enquiry is for a component fabricated from plate, send the drawing
and we will confirm the grade and the most economical supply route. Mill test
certificates to EN 10204 3.1, third party inspection and specific packaging
requirements can all be arranged on request.
For the same alloys in other forms, our
Nickel 200 and Nickel 201 seamless pipe and tube
covers ASME SB-161, and
Nickel 200 and Nickel 201 round bar, rod and wire
covers ASME SB-160. The
nickel alloy plate and sheet
category collects the rolled product forms, and the
material selection and properties
reference explains how the carbon difference translates into service life.